Milled Fiber
Milled fiber is made by cutting ARG fiber shortly into the length of dozens to several hundreds μm. Its high alkali and heat resistance is used as viscosity modifier for special paint.
Product Details
Property | Unit | |
---|---|---|
Thermal Expansion Coefficient | ×10-6/K | 9 |
Softening point | ℃ | 830 |
Density | ×103kg/m3 | 2.8 |
Tensile Strength | GN/m2 | 1.5 |
Young’s modulus | GN/m2 | 74 |
Strain to failure | % | 2 |
Alkali-resistivity, Weight loss (saturated cement solution, 80℃, 200 hours) |
% | ARG Fiber : 0.8 (E Glass Fiber:10.5) |
Acid-resistivity, Weight loss (10% HCl, 80℃, 90 hours) |
% | ARG Fiber : 1.6 (E Glass Fiber : 42.9) |
Acid-resistivity, Weight loss (10% H2SO4, 80℃, 90 hours) |
% | ARG Fiber : 1.2 (E Glass Fiber : 42.0) |
※The above values are only advisory, not guaranteed values.
Alkali-resistivityComparison of Alkali Erosive Attack(SEM-photographs) |
Acid-resistivityComparison of Acid Erosive Attack(SEM-photographs) |
||
ARG Fiber | ARG Fiber | ||
---|---|---|---|
Well-nigh perfect |
Well-nigh perfect |
||
E Glass Fiber | E Glass Fiber | ||
No trace of its original form |
Damaged at even intervals |